<listing id="vjp15"></listing><menuitem id="vjp15"></menuitem><var id="vjp15"></var><cite id="vjp15"></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><menuitem id="vjp15"></menuitem></video></cite>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<menuitem id="vjp15"><strike id="vjp15"></strike></menuitem>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"></strike></var>
<var id="vjp15"></var>
<var id="vjp15"></var>
<var id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></var>
<menuitem id="vjp15"></menuitem><cite id="vjp15"><video id="vjp15"></video></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></cite>
<var id="vjp15"></var>
<var id="vjp15"></var>
<menuitem id="vjp15"><span id="vjp15"><thead id="vjp15"></thead></span></menuitem>
<cite id="vjp15"><video id="vjp15"></video></cite>
<menuitem id="vjp15"></menuitem>

竹地板的制作方法與流程

文檔序號:12371031閱讀:來源:國知局

技術特征:

1.竹地板的制作方法,其特征在于,包括以下步驟:

步驟一 煮制

將竹地板原料放入添加有質量為所述竹地板原料的2%-4%的添加劑的水中,進行煮制,所述添加劑包括按重量份比例為6:3:2:3的牛皮膏、腰果酚、硫磺和硬脂酸鋅;

步驟二 加工

將經過步驟一處理的所述竹地板原料制成竹地板。

2.如權利要求1所述的竹地板的制作方法,其特征在于,煮制時間為50分鐘,煮制溫度為120℃。

3.如權利要求1所述的竹地板的制作方法,其特征在于,所述步驟一還包括將煮制好的竹地板原料進行碳化處理和烘干。

4.如權利要求1所述的竹地板的制作方法,其特征在于,所述步驟二包括:

將經過步驟一處理的所述竹地板原料依次進行切片成型、干燥施膠、熱壓成型和上漆處理制成所述竹地板。

5.如權利要求1所述的竹地板的制作方法,其特征在于,所述竹地板的尺寸為120cm*15.5cm*1.8cm。