<listing id="vjp15"></listing><menuitem id="vjp15"></menuitem><var id="vjp15"></var><cite id="vjp15"></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><menuitem id="vjp15"></menuitem></video></cite>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<menuitem id="vjp15"><strike id="vjp15"></strike></menuitem>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"></strike></var>
<var id="vjp15"></var>
<var id="vjp15"></var>
<var id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></var>
<menuitem id="vjp15"></menuitem><cite id="vjp15"><video id="vjp15"></video></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></cite>
<var id="vjp15"></var>
<var id="vjp15"></var>
<menuitem id="vjp15"><span id="vjp15"><thead id="vjp15"></thead></span></menuitem>
<cite id="vjp15"><video id="vjp15"></video></cite>
<menuitem id="vjp15"></menuitem>

一種制備儲氫物質鎂鎳合金納米纖維的方法與流程

文檔序號:11148381閱讀:1059來源:國知局
一種制備儲氫物質鎂鎳合金納米纖維的方法與制造工藝

本發明屬于氫氣存儲材料制備技術領域,具體涉及制備儲氫物質鎂鎳合金納米纖維的方法。



背景技術:

不可再生化石能源的大量消耗,人類生存環境的日益惡化換得了人類經濟的迅猛發展,能源是人類賴以生存、生產和生活的重要源泉,為了滿足全球對清潔能源的需求,解決日益嚴重的能源危機,尋找合適的可替代能源是各國的戰略目標。[1] 在各種可替代能源中,氫能因其儲量豐富,燃燒能量密度值高,燃燒產物(水)清潔無污染等一系列優勢成為最理想的二次能源。如何安全高效地儲存氫能是當前氫能應用的瓶頸問題。[2,3] 隨著氫經濟的發展,許多儲氫材料不斷被開發,如合金,輕金屬氫化物,碳納米管等。鎂基儲氫材料以其豐富的儲備,低廉的價格,以及容量高,可逆性好等特點而備受關注,但是它還存在高的吸放氫溫度和緩慢的動力學這兩個主要應用障礙,MgH2具有極高的熱力學穩定性,分解焓變高達74.6 KJ/(mol·H2)。放氫溫度往往在350 ℃以上,這限制了其在儲氫方面的實際應用,而通過與Ni,Cu,Al等合金化能夠改變MgH2的分解路徑,降低其熱力學穩定性,從而能夠顯著改善MgH2的熱力學性能,Ni作為一種廉價易得的金屬,其與Mg的二元合金產物Mg2Ni具有相對較高的理論含氫量(3.6 wt.%)和快速可逆吸放氫的性能受到廣泛研究。但是目前合成Mg2Ni的方法存在種種不足。比如常規的共熔法由于Mg的低熔點、高揮發性以及MgNi金屬間高的熔點差異受到限制很難制備高純度的Mg2Ni合金。[4-6]有研究表明機械球磨的方法可以合成Mg2Ni。[7-10]但是此法耗時長,并且最終產物均一性和純度會受到球磨轉速,球料比,球磨時間等多種因素的影響。此外,長的球磨時間容易使樣品發生氧化。為了解決這個問題,Sun課題組提出了兩步法合成Mg2Ni。先將Mg粉與Ni粉簡單球磨20 min后再在500 ℃,Ar氣氛下進行固相反應合成Mg2Ni。[11]但是此法步驟較為繁瑣。后來Li等人采用H等離子體法合成Mg,Ni納米顆粒,然后在4 MPa氫壓,350 ℃條件下,利用Mg,Ni納米顆粒反應合成Mg2NiH4,再經后續脫氫后便得到純Mg2Ni。[12,13]但此法引進了H等離子體設備,目前只能應用于實驗室合成,不適合工業化批量生產。本發明開創性的利用高溫熱蒸發法將Mg蒸發到Ni納米纖維表面進行原位反應制備Mg-Ni納米纖維。

參考文獻:

【1】. Schmitz, B., Virtual Reality: On the Brink of Greatness [J]. Computer Aided Engineering, Vol. 12, No. 4, 1993, pp.26~32.

【2】. Jayaram, S., Connacher, H.I., and Lyons, K.W., Virtual Assembly Using Virtual Reality Techniques [J]. Computer Aided Design, Vol. 29, No. 8, 1997, pp. 575~584.

【3】. Jung, B., Hoffhenke, M., and Wachsmuth, I., Virtual Assembly With Construction Kits [M]. Proceedings of 1997 ASME Design Engineering Technical Conference, September 14-17, 1997, Sacramento, DETC97/DFM-4363.

【4】. Hsu C-W, Lee S-L, Jeng R-R, Lin J-C. Mass production of Mg2Ni alloy bulk by isothermal evaporation casting process [J]. Int J Hydrogen Energy, 2007,32:4907-4911.

【5】. Sun D, Enoki H, Gingl F, Akiba E. New approach for synthesizing Mg-based alloys [J]. J Alloys Compd., 1999, 285:279-283.

【6】. Knight Jr L, Brittain R, Duncan M, Joyner C. Unusual behavior of vaporaized magnesium under low pressure conditions [J]. J Phys Chem., 1975, 79: 1183-1190.

【7】. Ebrahimi-Purkani A, Kashani-Bozorg SF, Nanocrystalline Mg2Ni-based powders produced by high-energy ball milling and subsequent annealing [J]. J Alloys Compd., 2008,456:211-215.

【8】. Simicic MV, Zdujic M, Dimitrijevic R, Nikolic-Bujanovic L, Popovic NH. Hydrogen absorption and elecdtrochemical properties of Mg2Ni-type alloys synthesized by mechanical alloying [J]. J Power Sources, 2006, 158: 730-734.

【9】. Zaluski L, Zaluska A, Stromolsen JO. Hydrogen absorption in nanocrystalling Mg2Ni formed by mechanical alloying [J]. J Alloys Compd., 1995, 217: 245-249.

【10】. Lee HY, Goo NH, Jeong WT, Lee KS. The surface state of nanocrystalline and amorphous Mg2Ni alloys prepared by mechanical alloying [J]. J Alloys Compd., 2000, 313: 258-262.

【11】. Zhao B, Fang F, Sun D, Zhang Q, Wei S, Cao F, er al. Formation of Mg2Ni with enhanced kinetics: Using MgH2 instead of Mg as a starting material [J]. J Solid State Chem., 2012, 192: 210-214.

【12】. Shao H, Liu T, Li X. Preparation of the Mg2Ni compound from ultrafine particles and its hydrogen storage properties [J]. Nanotechnology, 2003,14: L1-L3.

【13】. Shao HY, Liu T, Wang YT, Xu HR, Li XG. Preparation of Mg-based hydrogen storage materials from metal nanoparticles [J]. J Alloys Compd., 2008, 456: 527-533.。



技術實現要素:

本發明目的是提供一種工藝簡單的制備鎂鎳(Mg-Ni)合金納米纖維的方法。

本發明提供的制備鎂鎳合金納米纖維的方法,通過改變靜電紡絲法制備Ni(NO3)2/PVP纖維的煅燒條件,合成竹節狀的Ni納米纖維作為Ni源,利用高溫熱蒸發法將Mg蒸發到Ni納米纖維表面進行原位反應,制備得到Mg-Ni納米纖維。具體步驟為:

(1)用靜電紡絲法合成竹節狀的Ni納米纖維:

將溶有Ni(NO3)2和PVP的DMF/乙醇溶液用靜電紡絲法制備Ni(NO3)2/PVP纖維,然后,在管式爐中將Ni(NO3)2/PVP纖維在空氣中煅燒成NiO纖維,最后在H2/N2混合氣保護下將NiO纖維還原為Ni纖維;

(2)用熱蒸發法將Mg粉蒸發到Ni納米纖維表面:

將裝有Ni纖維的瓷舟置于鋪滿Mg粉的大瓷舟內,密封,然后在保護氣體Ar下,用管式爐對其煅燒,將Mg粉蒸到Ni納米纖維表面,并與Ni進行原位反應,生成Mg-Ni納米纖維。

本發明步驟(1)中,所述煅燒Ni(NO3)2/PVP纖維的條件為:以1~5 ℃/min速率升溫到190~220 ℃,保溫1~3 h;然后繼續以此速率升溫至500~550 ℃,在此溫度下保溫2~4 h;所述還原NiO纖維的條件為:H2/N2混合氣的保護下,以1~5 ℃/min速率升溫至380-420℃,在此溫度下保溫2~4 h,結束后冷卻至室溫。

本發明步驟(2)中,所述煅燒條件為:以1~5 ℃/min速率升溫至500 -550℃,隨即再從此溫度以2-3 ℃/min速率升溫至600~650 ℃,在此溫度保溫2~3h,然后冷卻至室溫。

本發明所合成的Mg-Ni合金納米纖維,由許多納米晶粒堆積而成,纖維尺寸在80-200 nm不等。

本發明所合成的Mg-Ni合金納米纖維是一中理想的儲氫物質,在氫壓30 bar,100 ℃下,100 min內即可吸附1.31 wt.%的氫氣;在235 ℃,1 min內吸氫量就能達到1 wt.%,總的儲氫容量為2.25 wt.%;吸完氫后,在265 ℃,1 min內能夠快速放出1.5 wt.%的氫氣,總放氫量為2.13 wt.%。

本發明具有以下幾個方面顯著優點:

(1)使用Mg-Ni合金納米纖維作為氫源材料,可于較低的加熱溫度下獲得大量高純氫氣;

(2)制備設備簡單,易于實現;

(3)工藝簡單,合成方便,成本適中。

附圖說明

圖1靜電紡絲法合成的NiO納米纖維(NiO NFs),還原后的Ni纖維(Ni NFs), Mg-Ni合金納米纖維(Mg-Ni NFs)的XRD圖。

圖2為NiO納米纖維、Ni納米纖維、Mg-Ni合金納米纖維的有關圖片。其中, a為 靜電紡絲法制備的NiO納米纖維的TEM照片;b為竹節狀的Ni納米纖維的TEM照片;c 為Mg-Ni合金納米纖維的TEM照片;d為Mg-Ni合金納米纖維的HRTEM照片;e為單根的TEM照片,f為e中元素Ni譜圖,g 為e中的元素Mg譜圖。

圖3 Mg-Ni合金納米纖維熱分解性能譜圖。其中,黑線,為Mg-Ni合金納米纖維的加氫產物的質譜圖;紅線為 Mg-Ni粉末樣品的加氫產物的質譜圖。

圖4產物吸放氫后的XRD譜圖,其中,a為Mg-Ni合金納米纖維吸氫后的產物;b 為Mg-Ni合金納米纖維放氫后的產物。

圖5 Mg-Ni合金纖維不同溫度條件下的吸氫曲線(上)。

圖6 Mg-Ni合金纖維不同溫度條件下的放氫曲線(下)。

具體實施方式

下面通過實施例進一步說明本發明。

實施例1:

1.Ni納米纖維的制備:共分為三步。首先,量取1.25 ml的DMF和乙醇,混合均勻。然后在混合的有機溶劑中,加入0.17 g的PVP,攪拌幾分鐘溶解,再加入0.101g的Ni(NO3)2·6H2O,繼續攪拌5 h后得到澄清的綠色溶液,用于靜電紡絲。參數設置:電壓12 KV,噴絲頭距接收板15 cm,液體流速為0.25 ml/h,在室溫條件下紡絲。第二步,將負極板上接受的Ni(NO3)2/PVP前驅纖維在空氣中煅燒得到NiO纖維。煅燒程序為1 ℃/min到190 ℃,保溫2 h后繼續升溫至500 ℃,保溫3 h。第三步,還原NiO纖維,在400 ℃,H2/N2混合氣的保護下保溫2 h,可以使NiO還原成Ni纖維。

2.Mg-Ni合金納米纖維制備:稱取Ni線25 mg于小瓷舟 A中,將瓷舟 A置于底部鋪滿Mg粉(400 mg) 大瓷舟 B內部,蓋上瓷舟蓋密封。將瓷舟 B移入石英管內,置于管式爐加熱,通保護氣體Ar。熱處理程序為:先5 ℃/min 到500 ℃,再以2 ℃/min到650 ℃保溫2 h,后冷卻至室溫。作為對比,稱取等量Ni粉按照相同方法合成Mg2Ni粉末樣品。

3.Mg-Ni納米纖維加氫過程:稱取20 mg樣品與高壓反應釜中,加入30 bar的氫壓,在300℃保溫5 h后冷卻至室溫。按照相同方法對合成的Mg-Ni粉末樣品進行加氫操作作為對比試驗。產物的XRD如圖1所示,合成產物的形貌表征如圖2所示,圖3為Mg-Ni納米纖維及其對比樣品的熱分解性能圖譜,而Mg-Ni納米纖維吸氫和放氫后的產物分析如圖4所示,最后,Mg-Ni納米纖維的吸放氫性能如圖5-6所示。

實施例2:

1.Ni納米纖維的制備:共分為三步。首先,量取2.5 ml的DMF和乙醇,混合均勻。然后在混合的有機溶劑中,加入0.34g的PVP,攪拌幾分鐘溶解,再加入0.202g的Ni(NO3)2·6H2O,繼續攪拌5 h后得到澄清的綠色溶液,用于靜電紡絲。參數設置:電壓12 KV,噴絲頭距接收板15 cm,液體流速為0.25 ml/h,在室溫條件下紡絲。第二步,將負極板上接受的Ni(NO3)2/PVP前驅纖維在空氣中煅燒得到NiO纖維。煅燒程序為3 ℃/min到220 ℃,保溫2 h后繼續以此速率升溫至550 ℃,保溫3 h。第三步,還原NiO纖維,在H2/N2混合氣的保護下,以5 ℃/min升到400 ℃,在400 ℃下保溫3 h,可以使NiO還原成Ni纖維。

2.Mg-Ni合金納米纖維制備:稱取Ni線25 mg于小瓷舟 A中,將瓷舟 A置于底部鋪滿Mg粉(400 mg) 大瓷舟 B內部,蓋上瓷舟蓋密封。將瓷舟 B移入石英管內,置于管式爐加熱,通保護氣體Ar。熱處理程序為:先5 ℃/min 到500 ℃,再以2 ℃/min到600 ℃保溫3 h,后冷卻至室溫。作為對比,稱取等量Ni粉按照相同方法合成Mg2Ni粉末樣品。

3.Mg-Ni納米纖維加氫過程:稱取20 mg樣品與高壓反應釜中,加入30 bar的氫壓,在300℃保溫5 h后冷卻至室溫。按照相同方法對合成的Mg-Ni粉末樣品進行加氫操作作為對比試驗。