<listing id="vjp15"></listing><menuitem id="vjp15"></menuitem><var id="vjp15"></var><cite id="vjp15"></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><menuitem id="vjp15"></menuitem></video></cite>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<menuitem id="vjp15"><strike id="vjp15"></strike></menuitem>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"></strike></var>
<var id="vjp15"></var>
<var id="vjp15"></var>
<var id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></var>
<menuitem id="vjp15"></menuitem><cite id="vjp15"><video id="vjp15"></video></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></cite>
<var id="vjp15"></var>
<var id="vjp15"></var>
<menuitem id="vjp15"><span id="vjp15"><thead id="vjp15"></thead></span></menuitem>
<cite id="vjp15"><video id="vjp15"></video></cite>
<menuitem id="vjp15"></menuitem>

小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法

文檔序號:3122733閱讀:287來源:國知局
小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法
【專利摘要】本發明公開了一種小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,用于解決現有小口徑管件內壁耐蝕堆焊接頭過熱而導致的焊接質量差的問題。本發明的焊接過程中焊有兩層焊層,其特征在于,第一層焊層時的焊接電流為110—120A,焊接電壓為25—30V,焊接速度為25—30cm/min;第二層焊層時的焊接電流為100—110A,焊接電壓為23—25V,焊接速度為25—30cm/min。本發明能夠防止焊接接頭過熱,從而防止產生粗大的柱狀晶粒,提高焊接的強度,防止裂紋的產生,從而提高焊接的質量。
【專利說明】小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法

【技術領域】
[0001]本發明涉及焊接領域,具體涉及一種小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法。

【背景技術】
[0002]隨著石油事業的蓬勃發展,以及我國石油戰略儲備工程的進行。工程工期要求緊,裝置中工作環境苛刻,管件內壁耐蝕堆焊要求越來越高,在各個工程中的需求也越來越大,最重要的是焊接質量的好壞直接影響整個工程的質量要求。
[0003]針對小口徑管件,由于其管徑的限制條件,所以只能采用明弧堆焊方法,熔化極氣體保護焊(GMAW)和非熔化極氣體保護焊(GTAW)兩種對焊方法。
[0004]鎳及鎳基合金具有獨特的物理、化學和耐蝕性能,同時在高溫和低溫下均具有良好的力學性能,因此鎳及鎳基合金在化學、石油、航天、航海和原子能等許多領域得到廣泛的運用。
[0005]然而,在堆焊的過程中由于鎳及鎳基合金焊縫金屬表面張力大,流動性差、粘性大不易成形和易產生氧化導致焊接質量差,并且成形的焊縫一般為凸狀,對于小口徑管件來說,凸狀的焊縫為影響管件的使用,甚至不能使用。
[0006]另外,由于鎳及鎳基合金導熱性差,現有的焊接工藝容易使焊接接頭過熱,產生粗大的柱狀晶粒,在粗大的柱狀邊界上,集中了低熔點共晶體,它們的強度低,脆性大,在焊接應力的作用下很容易形成裂紋,從而導致焊接質量差。


【發明內容】

[0007]本發明為解決上述技術問題,而提供一種小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,能夠防止焊接接頭過熱,從而防止產生粗大的柱狀晶粒,提高焊接的強度,防止裂紋的產生,從而提高焊接的質量。
[0008]與此同時,能夠改變焊接熔池的流動性,能夠改變鎳基合金焊接熔池的流動性、防止焊道被氧化,保證焊層的化學成分,從而提高焊接的質量,同時焊縫不會凸出,能夠滿足小口徑管件的焊接要求。
[0009]為解決上述問題,本發明所采用的技術方案是:
小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,其特征在于,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為110 — 120A,焊接電壓為25— 30V,焊接速度為25—30 cm/min ;第二層焊層時的焊接電流為100 — 110A,焊接電壓為23— 25V,焊接速度為25—30 cm/minο
[0010]第一層焊層焊接完成后,溫度冷卻至90度左右再進行第二層焊層的焊接,從而避免層間溫度過高的問題。
[0011]在焊接過程中,采用保護氣體進行保護,保護氣體的組份及組份的體積百分比為: 氬氣 90— 95%,
氦氣 5—10%。
[0012]所述氬氣的體積百分比為95%,所述氦氣的體積百分比為5%。
[0013]在焊接過程中,氬氣的氣體流量為20— 25 L/min。
[0014]焊接過程中,氬氣的氣體流量為20 L/min ο
[0015]焊接過程中,鎳基合金為ERNiCrMo-3,即為鎳基合金焊絲SNi6625。
[0016]與現有技術相比,本發明具有以下有益效果:
本發明的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,能夠防止焊接接頭過熱,從而防止產生粗大的柱狀晶粒,提高焊接的強度,防止裂紋的產生,保證焊接成型及焊縫的質量。
[0017]本發明焊接過程中,采用由體積百分比為90—95%的氬氣和5 —10%的氦氣組成的保護氣體進行焊接,能夠改變焊接熔池的流動性、防止焊道被氧化,保證焊層的化學成分,從而提高焊接的質量。同時使得焊縫不會凸出,保持焊道與管壁的平滑,能夠滿足小口徑管件的焊接要求。鎳基液體金屬的粘度及表面張力較大,流動性差,在保護氣體的吹動作用下,改善了金屬的流動性,焊縫成形良好。氬氣與氦氣是很強的惰性氣體,同時防止了液態鎳基金屬與空氣的化學反應,防止了氧化。
[0018]同時,在焊接的過程中,氬氣的氣體流量控制在20— 25L/min能夠啟到很好的保護作用。如果氣體流量小于20 L/min,不能達到保護的效果,外觀成型差;如果氣體流量大于25 L/min,產品制造成本增加,不可取。
[0019]本發明的鎳基合金為ERNiCrMo-3,該材料在惡劣的腐蝕環境中,有較寬的溫度范圍,并具有優良的抵抗小孔腐蝕和縫隙腐蝕的能力。從而提高耐腐蝕能力,提高管件的使用壽命。

【專利附圖】

【附圖說明】
[0020]圖1是本發明焊接過后的焊接示意圖;
圖2是不采用本發明焊接過后的焊接示意圖。

【具體實施方式】
[0021]下面結合實施例對本發明作進一步的描述,所描述的實施例僅僅是本發明一部分實施例,并不是全部的實施例。基于本發明中的實施例,本領域的普通技術人員在沒有做出創造性勞動前提下所獲得的其他所用實施例,都屬于本發明的保護范圍。
[0022]本發明的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為110 — 120A,焊接電壓為25— 30V,焊接速度為25—30 cm/min ;第二層焊層時的焊接電流為100 — 110A,焊接電壓為23— 25V,焊接速度為25—30 cm/minο
[0023]在進行焊接之前,對工件進行清理,保證焊件表面的清潔,是獲得鎳基合金優良堆焊層一個重要條件。工件表面上常有一層油脂、污垢與氧化物等,可以采用機械加工和化學清洗等工藝處理。
[0024]同時還需要對工件進行預熱處理,預熱的溫度為90— 100°C。鎳基合金流動性差,以免造成堆焊層表面成型差。
[0025]同時,在施焊過程中進行施焊時,采取短弧、快速焊,應控制層間溫度控制在90°左右,不超過100°c,線能量盡可能的小,第一層焊層的時候,線能量控制在8.6kj/cm以下,第二層焊層的時候,線能量控制在6.6kj/cm以下。鎳基合金焊接時熔池液態金屬的流動性差,熔深淺,要防止氣孔、未焊透等缺陷的產生。
[0026]本發明的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,能夠防止焊接接頭過熱,從而防止產生粗大的柱狀晶粒,提高焊接的強度,防止裂紋的產生,保證焊接成型及焊縫的質量。
[0027]在焊接過程中,采用保護氣體進行保護,保護氣體的組份及組份的體積百分比為:
氬氣 90— 95%,
氦氣 5—10%。
[0028]本發明的焊接過程中,選擇氬氣與氦氣的混合保護氣體能夠改變焊接熔池的流動性、防止焊道被氧化,保證焊層的化學成分,從而提高焊接的質量。同時使得焊縫不會凸出,保持焊道與管壁的平滑,能夠滿足小口徑管件的焊接要求。
[0029]鎳基液體金屬的粘度及表面張力較大,流動性差,在保護氣體的吹動作用下,改善了金屬的流動性,焊縫成形良好。氬氣與氦氣是很強的惰性氣體,同時防止了液態鎳基金屬與空氣的化學反應,防止了氧化。
[0030]作為一種優選的方式,IS氣的體積百分比為95%,所述氦氣的體積百分比為5%。
[0031]在焊接過程中,氬氣的氣體流量為20— 25 L/min。
[0032]焊接過程中,氬氣的氣體流量為20 L/min ο
[0033]在焊接過程中,氬氣的氣體流量為20—25 L/min,如果氣體流量小于20 L/min,不能達到保護的效果,外觀成型差;如果氣體流量大于25 L/min,產品制造成本增加,不可取。
[0034]作為本發明一種優選的方式,焊接過程中,氬氣的氣體流量為20 L/min。既能夠滿足焊接的外觀工藝要求,同時也能夠節約成本。
[0035]焊接過程中,鎳基合金為ERNiCrMo-3,即為鎳基合金焊絲SNi6625 ;該材料在惡劣的腐蝕環境中,有較寬的溫度范圍,并具有優良的抵抗小孔腐蝕和縫隙腐蝕的能力。從而提聞耐腐蝕能力,提聞管件的使用壽命。
[0036]實施例一
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為110A,焊接電壓為30V,焊接速度為25 cm/min ;第二層焊層時的焊接電流為110A,焊接電壓為23V,焊接速度為25 cm/min。本實施例焊接過后的焊縫示意圖如圖1所示。
[0037]實施例二
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為120A,焊接電壓為25V,焊接速度為30 cm/min ;第二層焊層時的焊接電流為100A,焊接電壓為25V,焊接速度為30cm/min。本實施例焊接過后的焊縫示意圖如圖1所示。
[0038]實施例三本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為115A,焊接電壓為28V,焊接速度為26 cm/min ;第二層焊層時的焊接電流為105A,焊接電壓為24V,焊接速度為27cm/min。本實施例焊接過后的焊縫示意圖如圖1所示。
[0039]實施例四
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為118A,焊接電壓為26V,焊接速度為29cm/min ;第二層焊層時的焊接電流為107A,焊接電壓為23.5V,焊接速度為28cm/min。本實施例焊接過后的焊縫示意圖如圖1所示。
[0040]實施例五
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為120A,焊接電壓為30V,焊接速度為30cm/min ;第二層焊層時的焊接電流為110A,焊接電壓為25V,焊接速度為30cm/min。本實施例焊接過后的焊縫示意圖如圖1所示。
[0041]實施例六
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為110A,焊接電壓為25V,焊接速度為25cm/min ;第二層焊層時的焊接電流為100A,焊接電壓為23V,焊接速度為25cm/min。本實施例焊接過后的焊縫示意圖如圖1所示。
[0042]實施例八
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為112A,焊接電壓為26V,焊接速度為27 cm/min ;第二層焊層時的焊接電流為101A,焊接電壓為24V,焊接速度為28 cm/min。焊接過程中,采用由體積百分比為90%的氬氣和10%的氦氣組成的保護氣體進行保護。本實施例焊接過后的焊縫示意圖如圖1所示,焊接的時候保持氬氣的氣體流量為20— 25 L/min。從外觀能夠看出,焊縫均勻、平滑,采用該組分組成的保護氣體進行焊接,焊接的外觀效果就好,滿足工藝要求。
[0043]焊接后進行彎曲測試,彎曲測試的表如下表所示:
^獅凝IfflMSIlI
warnBBB< }
麵彎》mi?.............................................................................................側奪wmiso卷傷...............................μ..........m.......................................................................10..................................................................................m...............................................................................1?................................................................................................................1imilim^...............................................................11...............................................................................................................................................................................................................................................m.........................................................................................................................................................................................................................................................................................................................................--.................................Μ1-lllllllllllllim~
再對耐蝕堆焊熔敷金屬化學成分(%)進行分析,分析結果如下表所示: 纔韁 C a Μι P S魏

MbMaMiz
要求——— —
?0Sii?
LOnBit ttiB ttJ5 HI? tOil a MS IftSS 175 621 ft ? Iil 1112 ft?
LSma IlOlI M2 Λ12 AOOK ft OiS IftiS &iS 62.C ?β -- 1112 ft25
2.0bbi ft ft 009 (LU ft 11 ft Mt ft OOS IftSO 142 623 ft 02 %M ft 12 <L2S
從表格分析能夠看出,焊接后的金屬化學成分,能達到實際需要要求。
[0044]實施例九
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為119A,焊接電壓為26V,焊接速度為26 cm/min ;第二層焊層時的焊接電流為102A,焊接電壓為23.5V,焊接速度為29 cm/min。焊接過程中,采用由體積百分比為95%的氬氣和5%的氦氣組成的保護氣體進行保護。本實施例焊接過后的焊縫示意圖如圖1所示,焊接的時候保持氬氣的氣體流量為20— 25 L/min。本實施例的焊縫均勻、平滑,采用該組分組成的保護氣體進行焊接,焊接的外觀效果就好,滿足工藝要求。
[0045]實施例十
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為112A,焊接電壓為26V,焊接速度為27 cm/min ;第二層焊層時的焊接電流為101A,焊接電壓為24V,焊接速度為28 cm/min。焊接過程中,采用由體積百分比為80%的氬氣和20%的氦氣組成的保護氣體進行保護。焊接的時候保持氬氣的氣體流量為20— 25 L/min。本實施例焊接過后的焊縫示意圖如圖2所示,焊接的外觀較差,焊縫凸出,不能滿足工藝要求。
[0046]焊接后進行彎曲測試,彎曲測試的表如下表所示:
一— immmΓΤΖΓΓΙΠ
?ηnm< }..............................?.........^.........................—...........................................10..................................................................................40...............................................................................180.................................................................................u ?rSmiS...............................1i"琢......................................................................................................................................................................................................11........................................................................?...............................................................................1i1......................................................Hi…1…~
~.........................1am....................................................................11...........................................................................................................................................................1?...............................1—~
彎曲測試滿足工藝要求。
[0047]焊接后,再進行金屬化學成分(%)分析,分析結果如下表所示:
mm c I a I* f s q m m m m- λ τ
IMmMu Mix
求—I— — — ——-— —
__MOai§
1.0mit <1isja 12 a 12 toil aow ?德鼇》sis q.m sue a 12 0.25
LStnft Il繼2| <114 flLil tOBl ft005 IftSS 4S7 S44 ft? 1S 敎 12 0.2S
?ββ 優 ft ill I ft 13 ft 15 ft OOl tt+flii IlSi SiS 512 ft? i 麵霾+H Λ?
從表中可以看出,本實施例焊接后的金屬化學成分分析不能達到實際需要要求,不能滿足工藝條件。
[0048]實施例^^一
本實施例的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為112Α,焊接電壓為26V,焊接速度為27 cm/min ;第二層焊層時的焊接電流為101A,焊接電壓為24V,焊接速度為28 cm/min。焊接過程中,采用由體積百分比為99%的氬氣和1%的氦氣組成的保護氣體進行保護。焊接的時候保持氬氣的氣體流量為20— 25 L/min。本實施例焊接過后的焊縫示意圖如圖2所示,焊接的外觀較差,焊縫凸出,不能滿足工藝要求。
[0049]焊接后進行彎曲測試,彎曲測試的表如下表所示:
ΞΓΓΤ1 MMPK II
圓誦ο..............................U.........每.....................................................................11........................................J........................................40...............................................................................1m..................................................................................側彎^..............................?~m....................................................................11.................................................................................?........................................1....................................1 藝.......................................................Hl.........................1? I 40 I i? ^
彎曲測試滿足工藝要求。
[0050]焊接后,再進行金屬化學成分(%)分析,分析結果如下表所示:
處暑 C S Mi F I S O- 1Α? N Qi Ie Jl I
~I■:::~IMnMn Ma
賽求 — — _ — I ———— —
[2M51Sf
LOnBiII aOIS 1112 ft 12 t1l Q._fi Ift40 ?56 SSf Λ 02 il? 1J2 O 25
LSue? Ife ft012 ft 14 ft II OLOOI I SQBS Ift35 &S7 5€4 霾 β i驪 ttJ2 (125
ZOaB n a ok a u ao aooi a ooe me ms Si 2 霾 e ±m 112 0.2s
不能達到實際需要要求。
[0051]實施例十二
本實施例的第一層焊層焊接電流不是110—12(^,焊接電壓不在25— 30V,焊接速度不在25— 30cm/min的時候,焊接的效果圖如圖2所示,不能滿足工藝條件。
[0052]實施例十二本實施例第二層焊層焊接焊接電流不在100 — 110A,焊接電壓不在23— 30V第二層焊層焊接速度不在25— 30cm/min的時候,焊接的效果圖如圖2所示,不能滿足工藝。
【權利要求】
1.小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,其特征在于,焊接過程中每一道焊縫具有兩層焊層,第一層焊層時的焊接電流為I1 — 120A,焊接電壓為25— 30V,焊接速度為25—30 cm/min ;第二層焊層時的焊接電流為100 — 110A,焊接電壓為23—25V,焊接速度為 25—30 cm/min。
2.根據權利要求1所述的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,其特征在于,在焊接過程中,采用保護氣體進行保護,保護氣體的組份及組份的體積百分比為: 氬氣 90— 95%, 氦氣 5—10%。
3.根據權利要求2所述的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,其特征在于,所述氬氣的體積百分比為95%,所述氦氣的體積百分比為5%。
4.根據權利要求2或3所述的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,其特征在于,在焊接過程中,氬氣的氣體流量為20— 25 L/min。
5.根據權利要求4所述的小口徑管件內壁熔化極鎳基合金耐蝕堆焊方法,其特征在于,焊接過程中,氬氣的氣體流量為20 L/min。
【文檔編號】B23K9/04GK104148788SQ201410451879
【公開日】2014年11月19日 申請日期:2014年9月5日 優先權日:2014年9月5日
【發明者】陳中均, 韋開棣, 李曉亮, 陳軒, 周鑫, 秦濤, 郭有田 申請人:四川石油天然氣建設工程有限責任公司
網友詢問留言 已有0條留言
  • 還沒有人留言評論。精彩留言會獲得點贊!
1
韩国伦理电影