<listing id="vjp15"></listing><menuitem id="vjp15"></menuitem><var id="vjp15"></var><cite id="vjp15"></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><menuitem id="vjp15"></menuitem></video></cite>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<var id="vjp15"><strike id="vjp15"><listing id="vjp15"></listing></strike></var>
<menuitem id="vjp15"><strike id="vjp15"></strike></menuitem>
<cite id="vjp15"></cite>
<var id="vjp15"><strike id="vjp15"></strike></var>
<var id="vjp15"></var>
<var id="vjp15"></var>
<var id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></var>
<menuitem id="vjp15"></menuitem><cite id="vjp15"><video id="vjp15"></video></cite>
<var id="vjp15"></var><cite id="vjp15"><video id="vjp15"><thead id="vjp15"></thead></video></cite>
<var id="vjp15"></var>
<var id="vjp15"></var>
<menuitem id="vjp15"><span id="vjp15"><thead id="vjp15"></thead></span></menuitem>
<cite id="vjp15"><video id="vjp15"></video></cite>
<menuitem id="vjp15"></menuitem>

一種1,3?二甲基?7?取代喹唑啉?2,4?二酮類化合物及其合成方法和應用與流程

文檔序號:11105204閱讀:1146來源:國知局
一種1,3?二甲基?7?取代喹唑啉?2,4?二酮類化合物及其合成方法和應用與制造工藝

本發明涉及化學合成技術領域,具體是一種1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物及其合成方法和應用。



背景技術:

目前研究發現,能夠引起人類疾病的真菌約有270種,可以感染人體的不同部位。淺部真菌僅侵犯人的皮膚、毛發、指甲等角化組織,而深部真菌能侵犯人的骨骼、內臟和中樞神經系統,呈現較高的發病率和死亡率。深度真菌感染已成為艾滋病、急性白血病、器官或骨髓移植等免疫抑制病人死亡的主要原因。隨著人類健康意識的提升及對真菌感染類疾病的重視,抗真菌藥物的研究已經成為全球藥物研究的一個熱點。盡管現在有大量的抗真菌藥物,如阿莫西林、兩性霉素B和唑類,但由于這些抗菌劑具有較窄的光譜活性,而且一些微生物已經產生抗藥性,因此,迫切需要設計合成新的抗菌藥物。

喹唑啉的環結構是多種生物堿的骨架。喹唑啉酮類藥物具有多重生物活性,近年來,喹唑啉酮類化合物在抗艾滋、抗腫瘤、抗癌、抗病毒、抗菌等方面的應用均有報道,這類化合物的研究文章可見:Eur J Med Chem.2009,3046-3055;Expert Opin Ther Pat..2015,789-804;American Journal of PharmTech Research.2013,466-475;Eur J Med Chem.2010,1200-1205;Chin J Chem.2003,339-346;International Research Journal of Pharmacy.2014,476-480;Prog Nat Sci.1998,359-365;Chem Biol Drμg Des.2015,672-684.

這些文獻均未覆蓋或包括本發明所涉及的新型化合物的結構、合成方法和用途。本發明設計合成了一類1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物。以多氧霉素B為對照,測定了新化合物對幾丁質合成酶的抑制作用,并測定了其在抗真菌,抗細菌方面的活性,拓展了喹唑啉的應用研究。到目前為止,本發明所涉及的新型化合物在抑制幾丁質合成酶活性方面還未見報道,所以將其作為幾丁質合成酶的抑制劑,開發成新型的抗真菌制劑,為人類的健康做出更大的貢獻。



技術實現要素:

本發明的目的在于提供一種1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物及其合成方法和應用,以解決上述背景技術中提出的問題。

為實現上述目的,本發明提供如下技術方案:

一種1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物,所述化合物的結構通式為:

式中R1為氫或乙基;R2為苯環、苯環衍生物、雜環或脂肪烴。

進一步的,所述化合物的結構為:

其中R1為H、CH2CH3;

R2為包括但不限于4-CH3OC6H4、4-CH3C6H4、4-FC6H4、4-ClC6H4、4-CF3C6H4、2-ClC6H4、CH2CH3。

進一步的,上述的1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物為下述化合物的任意一種,

一種所述的1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物的合成方法,按如下合成方式進行,

具體地說,上述反應條件如下

a)化合物1以DMF為溶劑,在堿性條件下和碘甲烷反應生成化合物2,進一步水解生成化合物3;

b)化合物3和尿素反應生成化合物4,再與碘甲烷反應生成化合物5,進一步水解得中間體6;

c)化合物7a-7u,分別與氯乙酰氯反應生成化合物8a-8u,8a-8u分別于N-甲基乙醇胺反應生成化合物9a-9u;

d)中間體6與化合物9a-9u,經縮合反應生成產物10a-10u。

作為本發明進一步的方案:具體步驟如下:

1)在反應器中,依次加入2-氨基對苯二甲酸二甲酯、氫氧化鈉、無水硫酸鈉、DMF為溶劑,室溫攪拌8~12min,再滴加碘甲烷與DMF的混合液,室溫反應55~65min,再加熱至50℃反應8~10h;

2)化合物2與氫氧化鈉的摩爾比為1:2~3,78~82℃反應1.5~2.5h,水和甲醇為溶劑;

3)化合物3與尿素摩爾比為1:9~11,145~155℃反應5~7h;

4)化合物4、碳酸鉀、碘甲烷、無水硫酸鈉摩爾比為1:1.8~2.2:1.8~2.2:0.2~0.3,DMF為溶劑,48~52℃反應8~10;

5)化合物5與氫氧化鈉摩爾比為1:9~11,48~52℃反應8~10,水和甲醇為溶劑;

6)化合物7a與氯乙酰氯、碳酸氫鈉摩爾比為1:1.1~1.3:4.5~5.5,二氯甲烷為溶劑,冰浴反應55~65min;

7)化合物8a、N-甲基乙醇胺、碳酸鉀摩爾比為1:1:1.4~1.6,乙腈為溶劑,78~82℃反應2h;

8)化合物6、9a-9u、DMAP、DCC的摩爾比為1:1:0.2~0.3:1,二氯甲烷為溶劑,冰浴反應1.5~2.5h。

一種所述的1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物在制備抗病原微生物藥物中的應用。

進一步的,所述微生物包括但不限于大腸桿菌、金黃色葡萄球菌、耐甲氧西林金黃色葡萄球菌、枯草桿菌、變形桿菌、銅綠色假單胞菌、白色念珠菌、新型隱球菌、黃曲霉菌、煙曲霉菌。

一種所述的1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物在幾丁質合成酶抑制劑藥物中的應用。

一種藥物組合物,其含有權利要求1、2所述的1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物和藥學上可接受載體。

與現有技術相比,本發明的有益效果是:

經生物活性測試實驗證明,本發明的部分化合物對白色念珠菌、黃曲霉菌、新型隱球菌和煙曲霉菌表現出較好的抑制活性。而且對幾丁質合成酶抑制活性明顯,抑菌效果較好,可用于制備抗病原微生物的藥物。

附圖說明

圖1為測試化合物濃度為300μg/ml時的幾丁質合成酶抑制率的對比圖。

具體實施方式

下面將結合本發明實施例中的附圖,對本發明實施例中的技術方案進行清楚、完整地描述,顯然,所描述的實施例僅僅是本發明一部分實施例,而不是全部的實施例。基于本發明中的實施例,本領域普通技術人員在沒有做出創造性勞動前提下所獲得的所有其他實施例,都屬于本發明保護的范圍。

實施例1

在帶有干燥管的250mL燒瓶中,加入2-氨基對苯二甲酸二甲酯(10.344g,50mmol),氫氧化鈉(3.000g,74mmol),無水硫酸鈉(1.776,12mmol)和二甲基甲酰胺(DMF)60mL,室溫攪拌十min后再滴加碘甲烷(10.508g,74mmol)與DMF 60mL的混合液,加畢室溫反應1h,再加熱至50℃反應9h,反應結束后,冷卻至室溫,加水100mL,用乙酸乙酯萃取(50mL×3),合并乙酸乙酯萃取液,無水硫酸鎂干燥,抽濾,濾液旋蒸除去溶劑,然后過柱(乙酸乙酯:石油醚=1:25),即制得化合物2(黃色固體)7.682g,收率68.9%,1H NMR(600MHz,CDCl3):δ3.49(s,3H,CH3),3.90(s,6H,CH3),7.00(s,1H,Ar-3-H),7.17(d,J=6.8Hz,1H,Ar-5-H),7.80(d,J=7.2Hz,1H,Ar-6-H);13C NMR(75MHz,CDCl3)δ:29.63,51.42,111.10,115.11,119.16,130.23,135.21,150.24,165.28,168.59;MS(m/z,%):224(M+1,100)。

實施例2

在250mL燒瓶中,加入化合物2(7.375g,33mmol)、水80mL、甲醇60mL和氫氧化鈉(3.330g,83mmol),加熱至80℃反應1h,反應結束后,旋蒸除去甲醇,用稀鹽酸調節pH=2,析出黃色固體,抽濾,濾餅用水洗滌(30mL×3)后干燥,即制得化合物3(黃色固體)5.920g,收率92%,1H NMR(600MHz,DMSO-d6):δ3.49(s,3H,CH3),7.77(d,J=8.1Hz,1H,Ar-5-H),7.83(s,1H,Ar-3-H),8.09(d,J=8.1Hz,1H,Ar-6-H),11.70(s,1H,COOH),13.58(s,1H,COOH);13C NMR(75MHz,CDCl3);δ29.63,111.76,112.16,119.14,130.22,134.21,150.29,166.38,169.52;MS(m/z,%):196(M+1,100)。

實施例3

在帶有干燥管的100mL燒瓶中,加入尿素(17.400g,290mmol),加熱至尿素完全溶解后,再加入化合物3(5.732g,29.mmol),加熱至150℃反應6h,反應結束后,冷卻至100℃,加水80mL,攪拌20min,冷卻至室溫,加鹽酸至PH=2,放置后抽濾,濾餅用水洗滌(50mL×3),干燥,即制得中間體4(肉色固體)5.742g,收率90.0%,1H NMR(600MHz,DMSO):δ3.49(s,3H,CH3)7.77(d,J=8.1Hz,1H,Ar-4-H),7.83(s,1H,Ar-6-H),8.09(d,J=8.1Hz,1H,Ar-3-H),11.70(s,1H,COOH),13.58(s,1H,COOH);13C NMR(75MHz,DMSO-d6)δ30.05,120,86,126.77,127.63,131.13,133.25,136.25,150.29,161.51,166.54;MS(m/z,%):221(M+1,100)

實施例4

在帶有干燥管的250mL燒瓶中,加入化合物4(4.400g,20mmol),碳酸鉀(2.760g,40mmol),DMF 40mL,無水硫酸鈉(0.710g,5mmol),室溫攪拌下緩慢向燒瓶中滴加碘甲烷5.680g,40mmol)與DMF 30mL的混合液,滴完后室溫反應1h,然后加熱至55℃反應6h,停止反應,冷卻至室溫,抽濾,濾液倒入200mL水中,攪拌,用乙酸乙酯萃取(50mL×4),硫酸鎂干燥乙酸乙酯層,抽濾,濾液旋蒸除去溶劑,得到淡黃色固體,用乙酸乙酯重結晶得到化合物5(白色松軟固體)4.072g,收率87.0%。1H NMR(600MHz,CDCl3):δ3.50(s,3H,CH3),3.67(s,3H,CH3),3.99(s,3H,CH3),7.90-7.87(m,2H,quinazolone-5,8-H),8.29(s,1H,quinazolone-6-H);13C NMR(75MHz,CDCl3):δ29.01,30.92,52.95,119.83,11.93,123.69,127.16,132.97,136.48,150.8,161.2,165.9;MS(m/z,%):249(M+1,100)。

實施例5

在250mL燒瓶中,加入化合物5(4.031g,16mmol)、水40mL、甲醇30mL和氫氧化鈉(6.400g,160mmol),加熱至60℃反應2h,反應結束后,旋蒸除去甲醇,用稀鹽酸調節pH=2,析出黃色固體,抽濾,濾餅用水洗滌(30mL×3)后干燥,即制得中間體6(黃色固體)3.440g,收率92%,1H NMR(600MHz,DMSO-d6):δ3.32(s,3H,CH3),3.57(s,1H,CH3),7.83(d,J=9.7Hz,2H,quinazolone-5,6-H),8.14(s,1H,quinazolone-8-H),13.55(s,1H,COOH).13C NMR(75MHz,DMSO-d6):δ29.0,30.95,120.81,120.93,126.62,127.13,131.93,136.42,150.8,161.2,165.9;MS(m/z,%):235(M+1,100)。

實施例6

在50mL圓底燒瓶中加入7a(0.456g,5mmol),CH2Cl2(10mL),碳酸氫鈉(1.050g,25mmol)室溫攪拌10min,冰浴滴加氯乙酰氯(0.672g,6mmol)的二氯甲烷(15mL)溶液,冰浴反應2h,停止反應,加水40mL,用二氯甲烷(15mL×3)萃取,合并有機層,用水(30mL×3)洗有機層,硫酸鎂干燥有機層,旋去溶劑得白色固體,用石油醚和乙酸乙酯混合溶劑重結晶得白色粉末狀固體8、化合物8b–8u的合成與8a相同.8a-8u的物理常數及光譜數據如下所示。

N-苯基-2-氯乙酰胺8a

白色粉末,產率89%,熔點141.4-142.6℃,1H NMR(600MHz,CDCl3):δ4.19(s,2H,CH2),7.19(t,J=7.4Hz,1H,Ar-4-H),7.36(t,J=7.7Hz,2H,Ar-3,5-H),7.55(d,J=8.1Hz,2H,Ar-2,6-H),8.26(s,1H,CONH);MS(m/z,%):170(M+1,100)。

N-(4-甲氧基苯基)-2-氯-乙酰胺8b

白色粉末,產率90%,熔點101.2-102.1℃,1H NMR(600MHz,CDCl3):δ3.68(s,3H,O-CH3),4.21(s,2H,CH2),6.86(d,J=9.1Hz,2H,Ar-3,5-H),7.46(d,J=9.1Hz,2H,Ar-2,4-H),8.23(s,1H,CONH);MS(m/z,%):200(M+1,100)。

N-(4-(三氟甲基)苯基)-2-氯-乙酰胺8c

白色針狀固體,產率92%,熔點161.2-162.3℃,1H NMR(600MHz,CDCl3):δ4.22(s,2H,CH2),7.62(d,J=12Hz,2H,Ar-3,5-H),7.69(d,J=9Hz,2H,Ar-2,4-H),8.36(s,1H,CONH);MS(m/z,%):238(M+1,100)。

N-(2-氯苯基)-2-氯-乙酰胺8d

粉色粉末,產率80%,熔點73.8–74.6℃,1H NMR(600MHz,CDCl3):δ4.21(s,2H,CH2),7.11(t,J=7.5Hz,1H,Ar-4-H),7.30(t,J=12.0Hz,1H,Ar-5-H,),7.36(d,J=9.1Hz,1H,Ar-3-H),8.47(d,J=6.2Hz,1H,Ar-6-H),8.94(s,1H,CONH);MS(m/z,%):204(M+1,100)。

N-(4-氯苯基)-2-氯-乙酰胺8e

白色針狀固體,產率82%,熔點180.4–181.3℃,1H NMR(600MHz,CDCl3):δ4.10(s,2H,CH2),7.22(d,J=9.1Hz,2H,Ar-3,5-H),7.53(d,J=12.0Hz,2H,Ar-2,4-H),8.27(s,1H,CONH);MS(m/z,%):204(M+1,100)。

N-(2-甲苯基)-2-氯-乙酰胺8f

白色粉末,產率84%,熔點109.7–111.1℃,1H NMR(600MHz,CDCl3):δ2.87(s,3H,CH3),4.18(s,2H,CH2),7.07(t,J=8.1Hz,1H,Ar-4-H),7.28(t,J=8.1Hz,1H,Ar-5-H),7.37(d,J=8.1Hz,1H,Ar-6-H),7.48(d,J=8.1Hz,1H,Ar-3-H),8.30(s,1H,CONH);MS(m/z,%):184(M+1,100)。

N-(4-甲苯基)-2-氯-乙酰胺8g

白色粉末,產率75%,熔點169.2–170.1℃,1H NMR(600MHz,CDCl3):δ3.43(s,3H,CH3),4.18(s,2H,CH2),6.90(d,J=8.1Hz,2H,Ar-3,5-H),7.56(d,J=8.7Hz,2H,Ar-2,4-H),8.30(s,1H,CONH);MS(m/z,%):184(M+1,100)。

N-(4-氟苯基)-2-氯-乙酰胺8h

白色針狀固體,產率83%,熔點129.9–131.0℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),7.22(d,J=9.1Hz,2H,Ar-3,5-H),7.63(d,J=12.0Hz,2H,Ar-2,4-H),8.27(s,1H,CONH);MS(m/z,%):188(M+1,100)。

N-(3-氯-4-氟苯基)-2-氯-乙酰胺8i

白色粉末,產率74%,熔點75.9–77.4℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),7.40(d,J=6.8Hz,1H,Ar-5-H),7.56(d,J=7.0Hz,1H,Ar-6-H),7.92(s,1H,Ar-2-H),8.28(s,1H,CONH);MS(m/z,%):222(M+1,100)。

N-(3-氯-4-甲基苯基)-2-氯-乙酰胺8j

白色粉末,產率90%,熔點176.7–178.0℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),7.40(d,J=6.8Hz,1H,Ar-5-H),7.58(d,J=7.0Hz,1H,Ar-6-H),7.82(s,1H,Ar-2-H),8.30(s,1H,CONH);MS(m/z,%):218(M+1,100)。

N-芐基-2-氯乙酰胺8k

粉色粉末,產率80%,熔點95.1–96.1℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),4.49(d,J=6.1Hz,2H,Ar-CH2),6.89(s,1H,CONH),7.29–7.38(m,5H,Ar-H);MS(m/z,%):184(M+1,100)。

N-(3-甲苯基)-2-氯-乙酰胺8l

白色粉末,產率86%,熔點90.2–91.1℃,1H NMR(600MHz,CDCl3),δ:2.37(s,3H,CH3),4.18(s,2H,CH2),6.97(d,J=8.1Hz,1H,Ar-4-H),7.28(t,J=8.1Hz,1H,Ar-5-H),7.37(d,J=8.1Hz,1H,Ar-6-H),7.48(s,1H,Ar-2-H),8.30(s,1H,CONH);MS(m/z,%):184(M+1,100)。

N-(3,5-二(三氟甲基)苯基)-2-氯乙酰胺8m

白色粉末,產率86%,熔點90.2–91.2℃,1H NMR(600MHz,CDCl3):δ4.23(s,2H,CH2),7.68(s,1H,Ar-4-H),8.17(s,2H,Ar-2,6-H),8.30(s,1H,CONH);MS(m/z,%):306(M+1,100)。

N-(4-硝基苯)-2-氯-乙酰胺8n

淡黃色粉末,產率88%,熔點190.6–191.8℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),7.26(d,J=6.2Hz,2H,Ar-3,5-H),8.63(d,J=9.0Hz,2H,Ar-2,6-H),8.27(s,1H,CONH);MS(m/z,%):215(M+1,100)。

N-(3,4-二氯苯基)-2-氯-乙酰胺8o

白色粉末,產率76%,熔點75.2–76.8℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),7.53(d,J=6.8Hz,1H,Ar-5-H),7.64(d,J=7.0Hz,1H,Ar-6-H),7.92(s,1H,Ar-2-H),8.28(s,1H,CONH);MS(m/z,%):238(M+1,100)。

2-(2-氯乙酰氨基)苯甲酸甲酯8p

白色粉末,產率80%,熔點98.3–99.4℃,1H NMR(600MHz,CDCl3):δ3.96(s,3H,CH3),4.22(s,2H,CH2),7.16(t,J=9.1Hz,1H,Ar-4-H),7.28(s,1H,CONH),7.57(t,J=7.5Hz,1H,Ar-5-H),8.06(d,J=3.2Hz,1H,Ar-3-H),8.70(d,J=9.5Hz,1H,Ar-6-H);MS(m/z,%):228(M+1,100)。

N-(6-甲氧吡啶)-2-氯-乙酰胺8q

白色粉末,產率72%,熔點127.6–128.2℃,1H NMR(600MHz,CDCl3):δ3.72(s,3H,CH3),4.26(s,2H,CH2),7.56(s,1H),8.28(s,1H,CONH),8.57(s,1H);MS(m/z,%):202(M+1,100)。

N-(1-萘)-2-氯-乙酰胺8r

白色粉末,產率68%,熔點162.3–163.1℃,1H NMR(600MHz,CDCl3):δ4.26(s,2H,CH2),6.89(d,J=6.7Hz,1H,naphthalen-2-H),7.37(t,J=7.3Hz,1H,naphthalen-3-H),7.44(t,J=7.6Hz,1H,naphthalen-7-H),7.54(t,J=8.0Hz,1H,Ar-6-H),7.66(d,J=5.1Hz,1H,naphthalen-4-H),8.03(d,J=5.1Hz,1H,naphthalen-5-H),8.15(d,J=8.0Hz,1H,naphthalen-8-H),9.86(s,1H,CONH);MS(m/z,%):220(M+1,100)。

N-乙基-2-氯-乙酰胺8s

淡黃色液體,產率75%,1H NMR(600MHz,CDCl3)δ:1.07(t,J=6.1Hz,3H,CH3),3.11(t,J=6.1Hz,2H,CH2),4.19(s,2H,CH2),8.08(s,1H,CONH);MS(m/z,%):122(M+1,100)。

N,N-二乙基-2-氯-乙酰胺8t

淡黃色液體,產率70%,1H NMR(600MHz,CDCl3)δ:1.17(t,J=6.2Hz,6H,CH3),3.47(t,J=6.2Hz,4H,CH2),4.19(s,2H,CH2);MS(m/z,%):150(M+1,100)。

N-叔丁基-2-氯乙酰胺8u

淡黃色液體,產率82%,1HNMR(600MHz,CDCl3):δ1.37(s,9H,CH3),4.19(s,2H,CH2),8.01(s,1H,CONH);MS(m/z,%):150(M+1,100)。

實施例7

在100mL圓底燒瓶中加入化合物8a(2.535g,15mmol),乙腈(40mL),K2CO3(3.105g,22.5mmol),滴加N-甲基乙醇胺(1.100g,15mmol)的乙腈(10mL)溶液,滴加完后60℃反應4h。反應結束后,減壓旋去乙腈,加入乙酸乙酯10mL,有機層用水洗至PH=7,取有機層,旋去溶劑得化合物9a。其他化合物9b–9u的合成方法同上。9a-9u的物理常數及光譜數據如下所示。

N-苯基-2-((2-羥基乙基)(甲基)氨基)乙酰胺9a

淡黃色液體,產率82%,1H NMR(600MHz,CDCl3):δ2.34(s,3H,CH3),2.64(t,J=5.4Hz,2H,CH2),3.32(s,2H,CH2),3.47(t,J=5.4Hz,2H,CH2),7.03(t,J=7.3Hz,1H,Ar-4-H),7.28(t,J=7.8Hz,2H,Ar-3,5-H),7.61(d,J=8.0Hz,2H,Ar-2,6-H),9.78(s,1H,CONH);MS(m/z,%):209(M+1,100)。

N-(4-甲氧基苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9b

淡黃色液體,產率85%,1H NMR(600MHz,CDCl3):δ2.50(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.32(s,2H,CH2),3.47(t,J=5.4Hz,2H,CH2),3.81(s,3H,CH3),7.08(d,J=7.8Hz,2H,Ar-3,5-H),7.51(d,J=8.0Hz,2H,Ar-2,6-H),9.36(s,1H,CONH);MS(m/z,%):239(M+1,100)。

N-(4-(三氟甲基)苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9c

黃色液體,產率86%,1H NMR(600MHz,CDCl3):δ2.60(s,3H,CH3),3.31(t,J=5.4Hz,2H,CH2),3.33(s,2H,CH2),3.47(t,J=5.4Hz,2H,CH2),7.10(d,J=7.8Hz,2H,Ar-3,5-H),7.51(d,J=8.0Hz,2H,Ar-2,6-H),9.75(s,1H,CONH);MS(m/z,%):277(M+1,100)。

N-(2-氯苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9d

淡黃色液體,產率85%,1H NMR(600MHz,CDCl3):δ2.52(s,3H,CH3),2.64(t,J=5.3Hz,2H,CH2),3.32(s,2H,CH2),3.47(t,J=5.4Hz,2H,CH2),7.03(t,J=7.5Hz,1H,Ar-4-H),7.17(t,J=7.8Hz,1H,Ar-5-H),7.53(d,J=7.6Hz,1H,Ar-3-H),8.02(d,J=8.0Hz,1H,Ar-6-H),9.75(s,1H,CONH);MS(m/z,%):243(M+1,100)。

N-(4-氯苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9e

淡黃色液體,產率82%,1H NMR(600MHz,CDCl3):δ2.63(s,3H,CH3),3.32(t,J=5.4Hz,2H,CH2),3.35(s,2H,CH2),3.47(t,J=5.4Hz,2H,CH2),7.37(d,J=8.0Hz,2H,Ar-3,5-H),7.63(d,J=7.6Hz,2H,Ar-2,6-H),9.69(s,1H,CONH);MS(m/z,%):243(M+1,100)。

N-(2-甲苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9f

淡黃色液體,產率88%,1H NMR(600MHz,CDCl3):δ2.12(s,3H,CH3),2.60(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.35(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),6.93(t,J=7.2Hz,1H,Ar-4-H),7.17(t,J=7.3Hz,1H,Ar-5-H),7.33(d,J=7.6Hz,1H,Ar-6-H),7.43(d,J=8.0Hz,1H,Ar-3-H),9.86(s,1H,CONH);MS(m/z,%):223(M+1,100)。

N-(4-甲苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9g

淡黃色液體,產率84%,1H NMR(600MHz,CDCl3):δ2.22(s,3H,CH3),2.44(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.32(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),7.11(t,J=8.2Hz,2H,Ar-3,5-H),7.46(t,J=8.3Hz,2H,Ar-2,6-H),9.76(s,1H,CONH);MS(m/z,%):223(M+1,100)。

N-(4-氟苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9h

淡黃色液體,產率82%,1H NMR(600MHz,CDCl3):δ2.16(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.31(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),7.12(t,J=7.6Hz,2H,Ar-3,5-H),7.50(t,J=7.7Hz,2H,Ar-2,6-H),9.85(s,1H,CONH);MS(m/z,%):223(M+1,100)。

N-(3-氯-4-氟苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9i

淡黃色液體,產率76%,1H NMR(600MHz,CDCl3):δ2.26(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.31(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),7.29(d,J=8.6Hz,1H,Ar-5-H),7.50(d,J=8.7Hz,1H,Ar-6-H),7.85(s,1H,Ar-2-H),9.73(s,1H,CONH);MS(m/z,%):261(M+1,100)。

N-(3-氯-4-甲基苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9j

淡黃色液體,產率83%,1H NMR(600MHz,CDCl3):δ2.23(s,3H,CH3),2.44(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.33(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),7.09(d,J=7.0Hz,1H,Ar-5-H),7.34(d,J=7.2Hz,1H,Ar-6-H),7.87(s,1H,Ar-2-H),9.85(s,1H,CONH);MS(m/z,%):257(M+1,100)。

N-芐基-2-((2-羥基乙基)(甲基)氨基)乙酰胺9k

淡黃色液體,產率70%,1H NMR(600MHz,CDCl3):δ2.60(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),,4.32(s,2H,CH2),3.47(t,J=5.4Hz,2H,CH2),4.31(s,2H,CH2),7.03(d,J=7.3Hz,2H,Ar-2,6-H),7.18(t,J=7.5Hz,1H,Ar-4-H),7.28(d,J=8.0Hz,2H,Ar-3,5-H),9.86(s,1H,CONH);MS(m/z,%):223(M+1,100)。

N-(3-甲苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9l

淡黃色液體,產率87%,1H NMR(600MHz,CDCl3):δ2.16(s,3H,CH3),2.24(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.31(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),6.92(d,J=5.0Hz,1H,Ar-4-H),7.24(t,J=7.2Hz,1H,Ar-5-H),7.42(d,J=5.0Hz,1H,Ar-6-H),7.64(s,1H,Ar-2-H),9.85(s,1H,CONH);MS(m/z,%):223(M+1,100)。

N-(3,5-二(三氟甲基)苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9m

淡黃色液體,產率76%,1H NMR(600MHz,CDCl3)δ:2.16(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.31(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),7.75(s,1H,Ar-4-H),8.14(s,2H,Ar-2,6-H),9.85(s,1H,CONH);MS(m/z,%):345(M+1,100)。

N-(4-硝基苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9n

淡黃色液體,產率67%,1H NMR(600MHz,CDCl3):δ2.26(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.32(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),7.82(t,J=8.0Hz,2H,Ar-2,6-H),8.24(t,J=7.7Hz,2H,Ar-3,5-H),9.85(s,1H,CONH);MS(m/z,%):254(M+1,100)。

N-(3,4-二氯苯基)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9o

淡黃色液體,產率77%,1H NMR(600MHz,CDCl3):δ2.23(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.34(s,2H,CH2),3.49(t,J=5.5Hz,2H,CH2),7.39(d,J=8.3Hz,1H,Ar-5-H),7.50(t,J=8.7Hz,1H,Ar-6-H),7.93(s,1H,Ar-2-H),9.85(s,1H,CONH);MS(m/z,%):277(M+1,100)。

2-(2-((2-羥基乙基)(甲基)氨基)乙酰氨基)苯甲酸甲酯9p

淡黃色液體,產率85%,1H NMR(600MHz,CDCl3):δ2.12(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.35(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),3.87(s,3H,CH3),7.20(t,J=7.2Hz,1H,Ar-4-H),7.47(t,J=7.3Hz,1H,Ar-5-H),7.83(d,J=7.6Hz,1H,Ar-3-H),8.23(d,J=8.0Hz,1H,Ar-6-H),9.86(s,1H,CONH);MS(m/z,%):267(M+1,100)。

N-(6-甲氧吡啶)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9q

淡黃色液體,產率67%,1H NMR(600MHz,CDCl3):δ2.16(s,3H,CH3),3.27(t,J=5.4Hz,2H,CH2),3.36(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),3.86(s,3H,CH3),7.46(s,1H,aromatic-H),9.30(s,1H,aromatic-H),9.85(s,1H,CONH);MS(m/z,%):241(M+1,100)。

N-(1-萘)-2-((2-羥基乙基)(甲基)氨基)乙酰胺9r

淡黃色液體,產率72%,1H NMR(600MHz,CDCl3):δ2.12(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.41(s,2H,CH2),3.47(t,J=5.5Hz,2H,CH2),6.89(d,J=6.7Hz,1H,naphthalen-2-H),7.37(t,J=7.3Hz,1H,naphthalen-3-H),7.44(t,J=7.6Hz,1H,naphthalen-7-H),7.54(t,J=8.0Hz,1H,Ar-6-H),7.66(d,J=5.1Hz,1H,naphthalen-4-H),8.06(d,J=5.1Hz,1H,naphthalen-5-H),8.13(d,J=8.0Hz,1H,naphthalen-8-H),9.86(s,1H,CONH);MS(m/z,%):259(M+1,100)。

N-乙基-2-((2-羥基乙基)(甲基)氨基)乙酰胺9s

淡黃色液體,產率79%,1H NMR(600MHz,CDCl3):δ1.04(t,J=6.7Hz,3H,CH3),2.12(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.31(s,2H,CH2),3.33(m,2H,CH2)3.47(t,J=5.5Hz,2H,CH2),8.86(s,1H,CONH);MS(m/z,%):161(M+1,100)。

N,N-二乙基-2-((2-羥基乙基)(甲基)氨基)乙酰胺9t

淡黃色液體,產率78%,1H NMR(600MHz,CDCl3):δ1.04(t,J=6.7Hz,6H,CH3),2.12(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.30(s,2H,CH2),3.34(m,4H,CH2),3.47(t,J=5.5Hz,2H,CH2);MS(m/z,%):189(M+1,100)。

N-叔丁基-2-((2-羥基乙基)(甲基)氨基)乙酰胺9u

淡黃色液體,產率79%,1H NMR(600MHz,CDCl3):δ1.34(s,9H,CH3),2.12(s,3H,CH3),3.29(t,J=5.4Hz,2H,CH2),3.32(s,2H,CH2),3.48(t,J=5.5Hz,2H,CH2),8.86(s,1H,CONH);MS(m/z,%):189(M+1,100)。

實施例8

在100mL圓底燒瓶中加入化合物6(1.200g,2.5mmol),CH2Cl2(15mL),DMAP(0.060g,0.003mmol),DCC(1.038g,2.5mmol),冰浴下滴加9a(1.045g,2.5mmol)的CH2Cl2(10mL)溶液,室溫反應6h。反應結束后,-15℃冷卻2h。過濾,干法過柱(乙酸乙酯:石油醚=1:1)得產物10a.化合物10b–10u合成方法同上。

上述制得的化合物,經X-6精密顯微熔點測定儀測定熔點(未校正);1H CNMR譜用BrukerAV-300型傅立葉變換核磁共振儀測定,使用Shimadzu LC-MS-2010A/EV測定,其具體分析數據如下:

白色粉末,產率68%,熔點156.5-157.3℃,1H NMR(600MHz,CDCl3):δ2.44(s,3H,CH3),2.93(t,J=5.0Hz,2H,CH2),3.20(s,2H,CH2),3.44(s,3H,CH3),3.48(s,3H,CH3),4.49(t,J=5.2Hz,2H,CH2),6.95(t,J=7.3Hz,1H,Ar-4-H),7.11(t,J=7.8Hz,2H,Ar-3,5-H),7.31(d,J=7.9Hz,2H,Ar-2,6-H),7.70(s,1H,CONH),7.76(d,J=8.1Hz,1H,quinolin-6-H),8.16(d,J=8.1Hz,1H,quinolin-5-H),8.93(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ29.81,30.80,43.52,58.06,61.64,62.28,119.63,119.92,121.68,125.64,127.59,128.03,128.91,133.72,136.15,138.58,151.30,161.92,165.93,168.52;MS(m/z,%):425(M+1,100)。

黃色粉末,產率80%,熔點133.3-134.8℃,1H NMR(600MHz,CDCl3):δ2.51(s,3H,CH3),2.98(t,J=4.7Hz,2H,CH2),3.25(s,2H,CH2),3.50(s,3H,CH3),3.51(s,3H,CH3),3.73(s,1H,CH3),4.55(t,J=5.2Hz,2H,CH2),6.68(d,J=8.7Hz,2H,Ar-3,5-H),7.24(d,J=8.8Hz,2H,Ar-2,6-H),7.73(s,1H,quinolin-8-H),7.86(d,J=8.1Hz,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),8.87(s,1H,CONH);13C NMR(75MHz,CDCl3):δ28.64,30.88,43.65,55.44,56.81,62.17,63.12,113.96,115.04,118.59,121.06,123.16,129.29,130.60,135.48,140.40,150.90,156.34,161.26,165.41,168.14;MS(m/z,%):455(M+1,100)。

黃色粉末,產率68%,熔點133.1-134.0℃,1H NMR(600MHz,CDCl3):δ2.54(s,3H,CH3),3.02(t,J=4.7Hz,2H,CH2),3.31(s,2H,CH2),3.49(s,3H,CH3),3.53(s,3H,CH3),4.58(t,J=5.2Hz,2H,CH2),7.42(d,J=8.5Hz,2H,Ar-3,5-H),7.53(d,J=8.4Hz,2H,Ar-2,6-H),7.73(s,1H,CONH),7.83(d,J=8.1Hz,1H,quinolin-6-H),8.26(d,J=8.1Hz,1H,quinolin-5-H),9.24(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ29.60,30.84,43.77,56.81,62.14,63.17,114.96,118.64,119.95,123.96,125.36,125.61,129.32,132.10,133.71,135.29,140.60,150.48,161.12,165.39,168.80;MS(m/z,%):493(M+1,100)。

黃色固體,產率68%,熔點197.8-199.0℃,1H NMR(600MHz,CDCl3):δ2.54(s,3H,CH3),3.02(t,J=5.0Hz,2H,CH2),3.29(s,2H,CH2),3.49(s,3H,CH3),3.53(s,3H,CH3),4.58(t,J=5.2Hz,2H,CH2),7.12(t,J=7.5Hz,1H,Ar-4-H),7.33(t,J=8.4Hz,1H,Ar-5-H),7.63(d,J=6.4Hz,1H,Ar-3-H),7.79(d,J=6.2Hz,1H,Ar-6-H),7.83(s,1H,CONH),7.96(d,J=8.1Hz,1H,quinolin-6-H),8.26(d,J=8.1Hz,1H,quinolin-5-H),9.24(d,J=8.1Hz,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ:28.63,30.84,43.77,56.81,62.14,63.20,114.96,118.64,118.95,123.06,125.96,129.32,135.29,140.60,150.48,161.12,165.39,168.80;MS(m/z,%):459(M+1,100)。

黃色粉末,產率77%,熔點135.4-136.7℃,1H NMR(600MHz,CDCl3):δ2.52(s,3H,CH3),2.99(t,J=5.2Hz,2H,CH2),3.26(s,2H,CH2),3.50(s,3H,CH3),3.51(s,3H,CH3),4.55(t,J=5.2Hz,2H,CH2),7.11(d,J=8.7Hz,2H,Ar-3,5-H),7.32(d,J=8.8Hz,2H,Ar-2,6-H),7.72(s,1H,CONH),7.82(d,J=8.1Hz,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),9.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ28.65,30.85,43.73,56.81,62.17,63.17,114.96,118.04,120.59,123.06,128.16,129.09,130.10,135.48,136.01,140.90,150.85,161.16,165.41,168.4;MS(m/z,%):459(M+1,100)。

白色粉末,產率79%,熔點130.3-131.5℃,1H NMR(600MHz,CDCl3):δ2.07(s,3H,CH3),2.56(s,3H,CH3),3.02(t,J=5.3Hz,2H,CH2),3.31(s,2H,CH2),3.49(s,3H,CH3),3.53(s,3H,CH3),4.56(t,J=5.3Hz,2H,CH2),6.97(t,J=7.5Hz,1H,Ar-4-H),7.03(t,J=7.3Hz,1H,Ar-5-H),7.15(d,J=7.4Hz,1H,Ar-6-H),7.74(s,1H,CONH),7.77(d,J=8.2Hz,1H,Ar-3-H),7.86(d,J=8.1Hz,1H,quinolin-6-H),8.16(d,J=8.1Hz,1H,quinolin-5-H),9.04(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ:17.43,28.63,30.84,43.77,56.81,62.14,63.20,114.96,118.52,121.95,123.06,124.96,126.32,127.29,129.20,130.60,135.39,139.44,140.30,150.48,161.12,165.39,168.80;MS(m/z,%):439(M+1,100)。

黃色粉末,產率80%,熔點137.6-139.0℃,1H NMR(600MHz,CDCl3):δ2.51(s,3H,CH3),2.64(s,3H,CH3),2.98(t,J=4.7Hz,2H,CH2),3.25(s,2H,CH2),3.50(s,3H,CH3),3.73(s,1H,CH3),4.55(t,J=5.2Hz,2H,CH2),7.21(d,J=8.7Hz,2H,Ar-3,5-H),7.44(d,J=8.8Hz,2H,Ar-2,6-H),7.73(s,1H,CONH),7.86(d,J=8.0Hz,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),8.87(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ21.64,30.88,43.65,55.44,56.81,62.17,63.12,113.96,115.04,118.59,121.06,123.16,129.29,130.60,135.48,140.40,150.90,156.34,161.26,165.41,168.14;MS(m/z,%):439(M+1,100)

黃色粉末,產率68%,熔點113.7-114.5℃,1H NMR(600MHz,CDCl3):δ2.39(s,3H,CH3),2.74(s,3H,CH3),2.86(t,J=4.7Hz,5H,CH2,CH3),3.16(s,2H,CH2),4.36(m,2H,CH2),,6.33(s,1H,CONH),6.85–6.79(m,2H,Ar-3,5-H),7.13(d,J=8.0Hz,2H,Ar-2,6-H),7.25(d,J=8.1Hz,1H,quinolin-6-H),7.36(d,J=8.1Hz,1H,quinolin-5-H),9.04(s,1H,quinolin-8-H);13CNMR(75MHz,CDCl3)δ28.60,30.84,43.77,56.81,62.14,63.17,114.96,119.63,119.91,120.35,125.69,127.64,133.75,134.11,136.12,151.38,161.97,162.95,165.85,168.53;MS(m/z,%):443(M+1,100)

黃色粉末,產率77%,熔點131.2-132.0℃,1H NMR(600MHz,CDCl3):δ2.26(s,3H,CH3),2.89(t,J=5.1Hz,2H,CH2),3.30(s,2H,CH2),3.36(s,3H,CH3),3.51(s,3H,CH3),4.65(t,J=5.1Hz,2H,CH2),7.11(d,J=8.6Hz,1H,Ar-5-H),7.23(s,1H,CONH),7.32(d,J=8.8Hz,1H,Ar-6-H),7.72(s,1H,quinolin-6-H),7.85(s,1H,Ar-2-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),9.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ28.65,30.85,43.73,56.71,62.23,63.17,114.96,118.04,119.90,120.59,123.06,124.21,125.63,127.65,133.10,135.48,136.01,149.90,154.85,161.16,165.41,168.48;MS(m/z,%):477(M+1,100)

黃色粉末,產率73%,熔點129.7-131.0℃,1H NMR(600MHz,CDCl3):δ2.26(s,3H,CH3),2.37(s,3H,CH3)2.89(t,J=5.1Hz,2H,CH2),3.30(s,2H,CH2),3.36(s,3H,CH3),3.51(s,3H,CH3),4.65(t,J=5.1Hz,2H,CH2),7.01(d,J=8.3Hz,1H,Ar-5-H),7.13(s,1H,CONH),7.32(d,J=8.8Hz,1H,Ar-6-H),7.64(s,1H,quinolin-6-H),7.85(s,1H,Ar-2-H),8.12(d,J=8.1Hz,1H,quinolin-5-H),9.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ26.72,28.65,30.85,43.73,56.71,62.23,63.17,114.96,118.04,120.59,123.06,128.16,129.09,130.10,135.48,136.01,138.90,150.85,161.16,165.41,168.48;MS(m/z,%):473(M+1,100)

白色粉末,產率79%,熔點158.2-159.7℃,1H NMR(600MHz,CDCl3):δ2.37(s,3H,CH3),2.83(t,J=5.0Hz,2H,CH2)3.03(s,3H,CH3),3.48(s,3H,CH3),,3.17(s,2H,CH2),4.33(t,J=5.2Hz,2H,CH2),4.38(d,J=6.2Hz,2H,CH2),6.87(s,1H,CONH),7.05(t,J=7.3Hz,1H,Ar-4-H),7.11(t,J=7.8Hz,2H,Ar-2,6-H),7.21(t,J=7.8Hz,2H,Ar-3,5-H),7.36(d,J=8.1Hz,1H,quinolin-6-H),7.48(d,J=8.1Hz,1H,quinolin-5-H),8.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ:28.65,30.85,43.73,44.67,56.71,62.23,63.17,114.96,118.04,120.59,123.06,128.16,129.09,130.10,135.48,136.01,138.90,150.85,161.16,165.41,168.48;MS(m/z,%):439(M+1,100)

黃色粉末,產率73%,熔點126.5-128.7℃,1H NMR(600MHz,CDCl3):δ2.31(s,3H,CH3),2.44(s,3H,CH3),2.98(t,J=4.7Hz,2H,CH2),3.25(s,2H,CH2),3.50(s,3H,CH3),3.73(s,1H,CH3),4.55(t,J=5.2Hz,2H,CH2),6.96(d,J=8.7Hz,1H,Ar-4-H),7.23(s,1H,CONH),7.31(t,J=8.6Hz,1H,Ar-2-H),7.64(d,J=8.0Hz,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),8.87(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ:21.64,28.36,30.88,43.65,56.81,62.17,63.12,118.96,119.04,119.59,121.06,123.16,124.53,128.06,129.29,135.48,137.21,138.56,150.90,160.34,161.26,165.41,168.14;MS(m/z,%):439(M+1,100)

黃色粉末,產率77%,熔點153.2-154.0℃,1H NMR(600MHz,CDCl3):δ2.26(s,3H,CH3),2.89(t,J=5.1Hz,2H,CH2),3.30(s,2H,CH2),3.26(s,3H,CH3),3.51(s,3H,CH3),4.67(t,J=5.1Hz,2H,CH2),7.23(s,1H,CONH),7.64(s,1H,Ar-4-H),7.72(s,1H,quinolin-6-H),8.12(s,2H,Ar-2,6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),9.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ28.65,30.85,43.73,56.71,62.23,63.17,114.96,118.04,120.59,123.06,124.4,128.16,129.09,130.10,135.48,136.01,149.90,150.85,161.16,165.41,168.48;MS(m/z,%):561(M+1,100)

黃色粉末,產率68%,熔點158.2-159.1℃,1H NMR(600MHz,CDCl3):δ2.63(s,3H,CH3),3.02(t,J=4.7Hz,2H,CH2),3.31(s,2H,CH2),3.49(s,3H,CH3),3.53(s,3H,CH3),4.58(t,J=5.2Hz,2H,CH2),7.73(s,1H,CONH),7.82(d,J=8.5Hz,2H,Ar-2,6-H),7.85(d,J=8.1Hz,1H,quinolin-6-H),8.14(d,J=8.4Hz,2H,Ar-3,5-H),8.26(d,J=8.1Hz,1H,quinolin-5-H),9.04(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3):δ28.60,30.84,43.77,56.81,62.14,63.17,118.96,118.64,119.05,123.06,125.96,129.32,135.29,144.60,150.48,161.12,165.39,168.80;MS(m/z,%):470(M+1,100)

黃色粉末,產率77%,熔點130.2-131.1℃,1H NMR(600MHz,CDCl3):δ2.47(s,3H,CH3),2.84(t,J=5.1Hz,2H,CH2),2.97(s,3H,CH3),2.98(s,3H,CH3),3.15(s,2H,CH2),4.65(t,J=5.1Hz,2H,CH2),6.92(s,1H,CONH),7.11(d,J=8.6Hz,1H,Ar-5-H),7.32(d,J=8.8Hz,1H,Ar-6-H),7.43(s,1H,quinolin-6-H),7.85(s,1H,Ar-2-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),9.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ28.65,30.85,43.73,56.71,62.23,63.17,115.06,117.64,118.79,119.86,123.16,129.49,130.10,131.60,134.01,135.90,136.25,140.28,151.45,161.16,165.41,168.48;MS(m/z,%):493(M+1,100)

白色粉末,產率79%,熔點138.5-139.7℃,1H NMR(600MHz,CDCl3):δ2.57(s,3H,CH3),3.01(s,2H,CH2),3.32(t,J=5.3Hz,2H,CH2),3.51(s,3H,CH3),3.59(s,3H,CH3),3.83(s,3H,CH3),4.66(t,J=5.3Hz,2H,CH2),7.01(t,J=7.5Hz,1H,Ar-4-H),7.50(t,J=7.3Hz,1H,Ar-5-H),7.74(s,1H,CONH),7.80(d,J=8.1Hz,1H,quinolin-6-H),7.87(d,J=8.2Hz,1H,Ar-3-H),8.16(d,J=7.4Hz,1H,Ar-6-H)),8.66(d,J=8.1Hz,1H,quinolin-5-H),10.04(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)28.63,30.84,43.77,51.5,56.81,62.14,63.20,115.36,119.52,121.95,123.06,124.26,126.32,127.29,129.20,133.60,136.39,139.44,141.30,149.48,161.12,165.39,168.80,169.20;MS(m/z,%):483(M+1,100)

黃色粉末,產率73%,熔點169.3-170.0℃,1H NMR(600MHz,CDCl3):δ2.31(s,3H,CH3),2.44(s,3H,CH3),2.98(t,J=4.7Hz,2H,CH2),3.25(s,2H,CH2),3.50(s,3H,CH3),3.73(s,1H,CH3),4.55(t,J=5.2Hz,2H,CH2),7.56(s,1H,Ar-6-H),7.64(d,J=8.0Hz,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),8.33(s,1H,CONH),8.87(s,1H,quinolin-8-H),9.01(s,1H);13C NMR(75MHz,CDCl3),δ:28.36,30.88,43.65,54.36,56.81,62.17,63.12,101.4,119.59,119.97,125.06,127.16,134.53,136.10,150.90,151.3,160.34,161.26,165.41,168.14,169.72;MS(m/z,%):457(M+1,100)

白色粉末,產率79%,熔點166.6-168.3℃,1H NMR(600MHz,CDCl3):δ2.67(s,3H,CH3),3.07(s,2H,CH2),3.15(s,3H,CH3),3.41(s,2H,CH2),3.50(s,3H,CH3),4.60(t,J=5.3Hz,2H,CH2),7.11(t,J=7.5Hz,1H,naphthalen-2-H),7.28(t,J=7.3Hz,1H,naphthalen-3-H),7.37(s,1H,CONH),7.40(t,J=6.3Hz,1H,naphthalen-5-H),7.48(d,J=8.1Hz,1H,quinolin-6-H),7.63(d,J=8.3Hz,1H,naphthalen-6-H),7.58(t,J=8.0Hz,1H,naphthalen-7-H),7.63(t,J=7.3Hz,1H,naphthalen-4-H),7.83(d,J=7.1Hz,1H,naphthalen-4-H),8.46(d,J=8.1Hz,1H,quinolin-5-H),9.62(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)28.63,30.84,43.77,58.5,62.14,63.20,105.36,119.02,119.65,119.91,121.02,124.26,125.32,125.69,126.20,127.31,128.59,133.60,134.39,135.44,136.30,151.12,161.39,165.80,168.20;MS(m/z,%):475(M+1,100)

黃色粉末,產率77%,熔點101.2-103.0℃,1H NMR(600MHz,CDCl3):δ1.04(t,J=7.1Hz,3H,CH3),2.47(s,3H,CH3),2.84(t,J=5.1Hz,2H,CH2),2.90(m,2H,CH2),2.97(s,3H,CH3),2.98(s,3H,CH3),3.15(s,2H,CH2),4.65(t,J=5.1Hz,2H,CH2),6.92(s,1H,CONH),7.43(s,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),9.03(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ15.70,29.65,30.85,33.86,43.73,58.71,62.03,63.17,119.56,119.90,125.16,127.49,133.10,136.60,151.45,161.16,165.41,168.48;MS(m/z,%):377(M+1,100)

黃色粉末,產率77%,熔點110.7-118.8℃,1H NMR(600MHz,CDCl3):δ1.24(t,J=7.1Hz,6H,CH3),2.47(s,3H,CH3),2.84(t,J=5.1Hz,2H,CH2),2.90(m,4H,CH2),2.97(s,3H,CH3),3.06(s,3H,CH3),3.15(s,2H,CH2),4.65(t,J=5.1Hz,2H,CH2),7.43(d,J=8.1Hz,1H,quinolin-6-H),8.23(d,J=8.1Hz,1H,quinolin-5-H),9.13(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ14.70,29.65,30.85,33.86,43.73,58.71,62.03,63.17,119.56,119.90,125.16,127.49,133.10,136.60,151.45,161.16,165.41,168.48;MS(m/z,%):405(M+1,100)

黃色粉末,產率77%,熔點104.7-105.6℃,1H NMR(600MHz,CDCl3):δ1.26(s,9H,CH3),2.47(s,3H,CH3),2.94(t,J=5.1Hz,2H,CH2),2.97(s,2H,CH2),3.51(s,3H,CH3),3.76(s,3H,CH3),4.65(t,J=5.1Hz,2H,CH2),7.07(s,1H,CONH),7.83(d,1H,J=8.1Hz,quinolin-6-H),7.90(d,J=8.1Hz,1H,quinolin-5-H),8.45(s,1H,quinolin-8-H);13C NMR(75MHz,CDCl3)δ29.20,29.65,30.85,33.86,43.73,58.71,62.03,63.17,119.56,119.90,125.16,127.49,133.10,136.60,151.45,161.16,165.41,168.48;MS(m/z,%):405(M+1,10

實施例9:1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物抗微生物活性實驗

本發明化合物用DMSO溶解后,用高壓滅菌的蒸餾水制成溶液備用,將96孔板,西林瓶,槍頭等物品高壓滅菌,用移液槍移取稀釋好的菌液溶液100uL到96孔板中,,用氧氟沙星,鏈霉素;氟康唑,多氧霉素B作為參比對照。細菌,真菌在37度培養24h,觀察現象。結果見附表。

附表1、本發明1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物抗細菌微生物活性數據(MICμg/mL)

附表2 1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物抗真菌微生物活性數據(MICμg/mL)

上述實驗以鏈霉素,氧氟沙星,氟康唑,多氧霉素B為對照藥,屬抗生素藥物,是公認的抗微生物活性很強的抗生素,但它目前已出現微生物耐藥現象。本發明新化合物無耐藥性,上述活性數據結果表明,本發明新化合物具有較明顯的抑菌作用,特別地,化合物10h對細菌均表現出顯著的抑制作用,其對變形桿菌MIC可達到64μg/mL,對大腸桿菌MIC可達到32μg/mL。化合物10l對真菌黃曲霉菌MIC可達到32μg/mL,優于多氧霉素B 64μg/mL。

實施例10:1,3-二甲基-7-取代喹唑啉-2,4-二酮類化合物幾丁質酶抑制活性實驗

幾丁質合成酶來源于啤酒酵母細胞膜,酶與底物在微孔板上一起孵化反應,產生的幾丁質與板上包被的WGA結合在一起而被固定,然后加入WGA-HRP,WGA-HRP可與固定在板上的幾丁質結合,將多余的試劑用蒸餾水洗掉,然后使用TMB底物溶液檢測HRP的活性,使用2M的硫酸終止反應后在450nm處檢測其OD,計算出化合物的IC50值。

其結果見附圖1。

對于本領域技術人員而言,顯然本發明不限于上述示范性實施例的細節,而且在不背離本發明的精神或基本特征的情況下,能夠以其他的具體形式實現本發明。因此,無論從哪一點來看,均應將實施例看作是示范性的,而且是非限制性的,本發明的范圍由所附權利要求而不是上述說明限定,因此旨在將落在權利要求的等同要件的含義和范圍內的所有變化囊括在本發明內。不應將權利要求中的任何附圖標記視為限制所涉及的權利要求。

當前第1頁1 2 3 
網友詢問留言 已有0條留言
  • 還沒有人留言評論。精彩留言會獲得點贊!
1
韩国伦理电影